Characteristics and basic shape of quenching cracks

Mar 21, 2024

Leave a message

During the quenching process, when the huge stress generated by quenching is greater than the strength of the material itself and exceeds the plastic deformation limit, cracks will occur. Quenching cracks often occur shortly after the mammal transformation begins. The distribution of cracks has no certain rules, but it is generally easy to form at the sharp corners and cross-section mutations of the workpiece.

The quenching cracking observed under the microscope may be intergranular cracking or transgranular cracking; some are radial, and some are separate lines or networks. Quenching cracks caused by excessive cooling in the martensitic transformation zone are often distributed transgranularly, and the cracks are true, with small cracks without branches around them. Quenching cracks caused by excessive quenching heating temperature are distributed along the grain, with sharp crack ends, and show overheating characteristics: coarse acicular martensite can be observed in structural steel; eutectic can be observed in tool steel. or angular carbides. High carbon steel workpieces with surface decarburization are prone to form network cracks after quenching. This is because the volume expansion of the surface decarburized layer during quenching and cooling is smaller than that of the non-decarburized core, and the surface material is pulled into a network shape by the expansion of the core.
The basic forms of quenching cracks mainly include: longitudinal cracks, transverse cracks, network cracks and peeling cracks, etc. The specific conditions are analyzed as follows:

1. Longitudinal cracks mostly occur on hardened steel parts, and they can only appear when the tangential tensile stress on the surface is greater than the axial tensile stress. This kind of cracks are distributed along the axial direction, from the surface crack to the center.

2. Transverse cracks occur in the transition zone between the hardened layer and the unhardened core when the workpiece is not hardened. The characteristic of internal stress is that the surface is compressed, and the compressive stress changes to tensile stress at a certain distance from the surface. The axial tensile stress is the largest, resulting in transverse cracks.

3. Stress concentration: Parts with angles, cuts, and grooves on cracked parts are prone to stress concentration. Coupled with uneven quenching and cooling, cracks are often caused in these parts. This kind of crack has no fixed morphological characteristics.

4. Reticular cracks are surface cracks with shallow depth, generally in the range of 0.01-2mm. The cracks can be oriented in any direction to form a reticular shape. After the surface of high-carbon steel workpiece is decarburized, its martensite specific volume is smaller, thus forming tensile stress on the surface, resulting in network cracks.

5. Peeling cracks occur in extremely thin areas where stress transitions sharply, and surface peeling occurs when internal cracks lurking parallel to the surface expand severely.

Send Inquiry